Accession Number : ADA953778

Title :   Examination of Defective 1-1/4 Inch Disston Face Hardened Plate,

Corporate Author : WATERTOWN ARSENAL LABS MA

Personal Author(s) : Reed,E. L. ; Kruegel,S. L.

Report Date : 23 MAY 1938

Pagination or Media Count : 15

Abstract : The purpose of this investigation was to determine the cause of failure of a 1-1/4 inch Disston Face Hardened Plate. Contributing causes of failure are: occasional bad laminations in steel base, coarse martensite near junction of case and core, indications of grain boundary carbide in core, considerable decarburization of case, and the use of a steel base with too high carbon content.

Descriptors :   *Armor plate, Hardness, Failure, Defects(Materials), Hardening, Carbon, Martensite, Carbides, Grain boundaries, Steel

Subject Categories : Armor